Journal of Korean Dental Association

Search

Close

J Korean Dent Assoc. 1985;23(7):577-583. Published online July 31, 1985.
반복 사용된 치과용 비귀금속에 의한 주조체의 식각표면에 대한 연구
이선형
서울대학교 치과대학 보철학교실
The Etched Surface of the Repeatedly Cast Dental Base Metal Alloy
Sun-Hyung Lee
Dept. of Prosthodontics, College of Dentistry Seoul National University
Abstract
The purpose of this investigation was to evaluate scanning electron micrographs of repeatedly cast base metal alloy. For this study two Ni-Cr-Be alloys were used; Rexillium III and Verabond. They were repeatedly cast without addition o new alloy melting with an electric resistant furnace (Castron 8, Yoshida dental equipment Mfg.Co.). They were etched with 10% H₂SO₄ Sol. at 300mA/㎠ for 3 minutes with the use of metal etching unit Oxyetch (OXY dental product Inc.), and ultrasonic cleaning in 18% HC1 Sol. was done. Etched surfaces were examined under a SEM at x 200 and x 750. The surfaces are shown in legends.

Keywords :